[AR] Re: APCP properties, was Re: Re: starship abort?

  • From: roxanna Mason <rocketmaster.ken@xxxxxxxxx>
  • To: arocket@xxxxxxxxxxxxx
  • Date: Sun, 30 Apr 2023 11:00:19 -0700

3. Added more AP to get to 88%. Qmodal AP: 600, 400, 200, 90 & Under.

Brian, Was this designed or just some stuff you had in your stock because
the devil is in the details and that "90 & under, may have some fines that
change the rheological properties significantly as in your description.
Have or can you do a sieve analysis and see if you have some <20u particles
in there that are fitting just right in between the larger particles. Ray
used the analogy of a bucket full of various sized items such as baseballs,
golfballs, marbles and BB's to illustrate how particles fit intricately
interlaced that by adding subsequent balls the height of the bucket doesn't
chant even though its weight continues to rise. I've seen solid loadings
upto 92% which sounds incredible but this is the reward for such research.
Every % over 90% is a real challenge. Your use of lecithin is interesting
because it seems like it's acting more like a surfactant than a
simple plasticizer. I used to use Tween 85 as a surfactant for aluminized
JP-8 in a water cooled GOx engine. The Tween worked great allowing high
solids while maintaining free flowing of the slurry through the injector.
As you mentioned scientists and chemists spend their lives experimenting
with these phenomena to extract maximum loading efficiencies especially in
sub launched  ICBMs and space motors like the Star and IUS to maximize
performance and space utilization.
Anyway, good work and good luck,

Ken

On Sun, Apr 30, 2023 at 12:48 AM BrianK ABQ <cielobenazul@xxxxxxxxx> wrote:

Ken,

I can't find that notebook so I'm working off memory here.

1. I usually made an 84% to 85% solids motor. Trimodal AP: 400, 200, 90 &
Under. 5% Al. They were quite reliable and reproducible.

2. For the 88% solids I added Lecithin (0.5%). Didn't use in my normal
motors.

3. Added more AP to get to 88%. Qmodal AP: 600, 400, 200, 90 & Under.

4. Had quite the "phase transition" in viscosity. After mixing for a while
it changed into a much less viscous fluid. And stayed that way through
casting.

That's all the detail I recall.

Cheers,

Brian

On Sun, Apr 30, 2023 at 1:12 AM roxanna Mason <rocketmaster.ken@xxxxxxxxx>
wrote:

That's a decent solids loading Brian, perhaps the lecithin acted as a
surfactant. Was this a single, bi or even trimodal?

Ken

On Sat, Apr 29, 2023 at 11:05 PM BrianK ABQ <cielobenazul@xxxxxxxxx>
wrote:

I briefly encountered some viscosity issues. I was trying to make some
small batch APCP with 88% solids. I recall two things.

1. A little lecithin (0.5%?) made a big difference.

2. After adding all the AP the mix really thickened. But after a bit of
mixing (20 min or so) the mix suddenly thinned and was fine to make motors
with.

Those behaviors are very finicky and formula dependent.

Cheers,

Brian


Other related posts: